USE OF WASTE PLASTIC IN CONCRETE
PAVERS
GUIDED BY BY:- PRESENTED BY:-
PROF. V. K. RAHMAN NABEEL KHAN INAMDAR
INTRODUCTION
Increasing Consumption.
5 million tones in 1930 to 100 million
tones in recent times.
Hazardous to environment.
Recycling.
20% only is recycled.
Disposing problem.
Decrease the amount of plastic for longer
time.
2
APPLICATION
CEMENT
OPC 43 Grade
cement is used.
SAND
Sand retaining on
2.5mm sieve.
4
COARSE
AGGREGATE
Responsible for
compressive strength.
Retaining on 4.75 mm
sieve is taken.
PLASTIC
AGGREGATE.
Replacement for coarse
aggregate.
Retaining on 4.75 mm
sieve.
5
LOW DENSITY
POLYETHYLENE
(LDPE).
Thermoplastic from
monomer ethylene.
POLYETHYLENE
TEREPTHALATE
(PET)
Thermoplastic polymer
resin.
Use of PET in bottles is
50% of total use of PET.
6
METHODOLOGY
7
Table :- Mix proportion of M40 Concrete
Cement 10 10 10 10
Sand 26 26 26 26
Total 33 33 33
8
TESTS
COMPRESSIVE STRENGTH
Where,
Fb= Flextual strength.
P= Applied load.
L= Length of specimen.
b=Width of specimen.
x=Depth of specimen.
10
TENSILE SPLITTING STRENGTH
ASTING OF SPECIMEN
Where,
P = Load at Failure
D = Dia. Of Specimen.
L = Length of Cylinder.
11
RESULTS
COMPRESSION TEST RESULTS
28 Days Average
Plastic
Strength(KN/m2 Strength(KN/m2
Aggregate in %
) )
39.50
0.00 42.00 41.10
41.00
39.00
10.00 40.30 40.07
40.90
38.70
20.00 39.60 38.97
38.60
37.60
30.00 38.60 37.77
12
FLEXURAL STRENGTH RESULT
6
FLEXURAL STRENGTH 3
0
0 10 20 30 40 50
% PLASTIC AGGREGATE
13
TENSILE SPLITTING TEST RESULT
4
3.5
SPLIT TENSILE STRENGTH
3
2.5
1.5
0.5
0
0 10 20 30 40 50
% OF PLASTIC AGGREGATE
14
CONCLUSION
15
REFERENCES
[1]Ganesh Tapkire, Satish Parihar, Pramod Patil, Hemraj
Kumavat, " Recycled Plastic used in Concrete Paver Block"
International Journal of Research in Engineering and
Technology(IJRET), Vol:3 June-2014 , pISSN:2321-7308