Comparable standards SKD11
Chemical composition C Si Mn Cr Mo V
(Typical analysis %) 1.47 0.25 0.40 11.80 1.00 0.30
Steel properties High wear resistance. Very good toughness, compression
strength and dimensional stability. Possibility of nitriding.
Physical properties Thermal conductivity W/(m.K) 20oC
20
3
Density g/cm 20oC
7.70
Coefficient of linear thermal expansion
-6 o -1 20-100 20-200 20-300 20-400 20-500 20-600 20-700oC
10 C 10.3 11.7 11.8 12.5 12.8 13.1 13.3

Applications High performance cutting tools, stamping, woodworking,


drawing, deep drawing and pressing tools, for ceramics and
pharmaceutical industries, rolls, measuring tools, plastic
moulds, shear blades.
Toughness is better than OCR12 (AISID3).
Stress Relieving 0
Holding at approx 650-700 C for one hour.
Heat treatment Soft annealingoC Cooling Hardness HB
840 - 880 furnace max. 240
o
Hardening from C in Hardness after quenching HRC
1010 - 1050 oil, air, thermal bath 62 - 64
500 - 550oC
o
Tempering C 100 200 300 400 500 525 550 600 700
HRC 63 60 58 58 60 58 55 46 35
Time - Temperature - Transformation - Diagram Tempering Diagram
70

65

60

55

50

45

40

35

30
0 100 200 300 400 500 600 700
Tempering Temperature in oC, Time 1.5 h