Documenti di Didattica
Documenti di Professioni
Documenti di Cultura
C2 P2 P1 C1
a
20
a a a
Position 3 Position 4
a (m) 2pa (m) R (W) R (W) R (W) R (W)
C2-P2-P1-C1 P2-C2-C1-P1 R (W) C2-P2-P1-C1 P2-C2-C1-P1 R (W)
0.5 3.14
1 6.28
2 12.57
4 25.13
8 50.27
16 100.53
32 201.06
64 402.12
0.00
0.00
0.00
0.00
Resistivity-Depth Curve
100
Position 1
Position 2
10 Depth Average 1 & 2
Position 3
Position 4
Column AQ
1
0.1 1
Spacing (Depth in metres)
1/2piR Vs Depth
12
10
8
1/2piR
Position 1
6 Position 2
Position 3
Position 4
0
Page 3 of 10 Form SP0522C01 Ver 1
0.4 0.5 0.6 0.7 0.8 0.9 1
Ergon Energy Corporation Limited ABN 50 087 646 06 2
Depth (m)
Position 4
0
0.4 0.5 0.6 0.7 0.8 0.9 1
Depth (m)
DETERMINATION OF UPPER LAYER THICKNESS & RESISTIVITIES FROM 1/(2pR) Vs DEPTH GRAPH
(Refer to SWP for direction)
Upper layer thickness from average curve (where the slope changes) 10
umber
ρ Average
(Wm)
ρ Average
(Wm)
sition 1
sition 2
pth Average 1 & 2
sition 3
sition 4
lumn AQ
Position 1
Position 2
Position 3
Position 4
PTH GRAPH
ohm-m
ohm-m
ssed: