Heat Resistant Steel

Casting Materials
material delivery ASTM delivery technological properties (at room temperature) max. operation
JUNKER DIN-number specification A297 condition Rp 0.2 Rm A5 temperature
[N/mm²] [N/mm²] [%] [°C]
F1002S 1.4743 DIN EN 10295 - not annealed3) - - - 900
AF1101 1.4823 DIN EN 10295 HD not annealed3) ≥ 250 ≥ 550 ≥3 1100
UNS J93005
A1050 1.4825 DIN EN 10295 HF not annealed ≥ 230 ≥ 450 ≥ 15 900
UNS J92603
A1201 1.4848 DIN EN 10295 HK not annealed ≥ 220 ≥ 450 ≥8 1100
UNS J94224
A1224Nb 1.4855 DIN EN 10295 - not annealed ≥ 220 ≥ 450 ≥4 1050
A1234Nb 1.4859 DIN EN 10295 - not annealed ≥ 180 ≥ 440 ≥ 20 1050
A1237 1.4857 DIN EN 10295 HP not annealed ≥ 220 ≥ 440 ≥6 1100
UNS N08705
A1205 2.4879 DIN EN 10295 - not annealed ≥ 240 ≥ 440 ≥3 1150
Thermco 50 2.4778 DIN EN 10295 - not annealed ≥ 235 ≥ 490 ≥6 12001)
G-NiCr50Nb 2.4680 DIN EN 10295 - not annealed ≥ 230 ≥ 540 ≥8 10502)
G-NiCr15 2.4815 DIN EN 10295 - not annealed ≥ 200 ≥ 400 ≥8 1100
(9.4816)
) For cyclical heatings. the maximum temperature is 1100°C in air.
1

) This alloy will be applied up to a maximum operation temperature of 950°C under conditions with oil-ash-influence.
2

) These alloys also can also be deliverd in annealed condition.


3
Heat Resistant Steel
Casting Materials
material analysis (%)
JUNKER DIN- C Si Mn P S Cr Mo Ni Nb other
number elements
F1002S 1.4743 1.40 - 1.80 1.00 - 2.50 ≤ 1.00 ≤ 0.040 ≤ 0.030 17.00 - 19.00 ≤ 0.50 ≤ 1.00 - -
AF1101 1.4823 0.30 - 0.50 1.00 - 2.50 ≤ 1.50 ≤ 0.040 ≤ 0.030 25.00 - 28.00 ≤ 0.50 3.00 - 6.00 - -
A1050 1.4825 0.15- 0.35 0.50 - 2.50 ≤ 2.00 ≤ 0.040 ≤ 0.030 17.00 - 19.00 ≤ 0.50 8.00 - 10.00 - -
A1201 1.4848 0.30 - 0.50 1.00 - 2.50 ≤ 2.00 ≤ 0.040 ≤ 0.030 24.00 - 27.00 ≤ 0.50 19.00 - 22.00 - -
A1224Nb 1.4855 0.30 - 0.50 1.00 - 2.50 ≤ 2.00 ≤ 0.040 ≤ 0.030 23.00 - 25.00 ≤ 0.50 23.00 - 25.00 0.80 - 1.80 -
A1234Nb 1.4859 0.05 - 0.15 0.50 - 1.50 ≤ 2.00 ≤ 0.040 ≤ 0.030 19.00 - 21.00 ≤ 0.50 31.00 - 33.00 0.50 - 1.50 -
A1237 1.4857 0.30 - 0.50 1.00 - 2.50 ≤ 2.00 ≤ 0.040 ≤ 0.030 24.00 - 27.00 ≤ 0.50 33.00 - 36.00 - -
A1205 2.4879 0.35 - 0.55 1.00 - 2.00 ≤ 1.50 ≤ 0.040 ≤ 0.030 27.00 - 30.00 ≤ 0.50 47.00 - 50.00 - W: 4.00 - 6.00
Fe: bal.
Thermco 50 2.4778 0.05 - 0.25 0.50 - 1.50 ≤ 1.50 ≤ 0.040 ≤ 0.030 27.00 - 30.00 ≤ 0.50 ≤ 4.00 ≤ 0.50 Co: 48.0 - 52.0
Fe: bal.
G-NiCr50Nb 2.4680 ≤ 0.10 ≤ 1.00 ≤ 0.50 ≤ 0.020 ≤ 0.020 48.00 - 52.00 ≤ 0.50 bal. 1.00 - 1.80 Fe: ≤ 1.00
N: ≤ 0.16
G-NiCr15 2.4815 0.35 - 0.65 1.00 - 2.50 ≤ 2.00 ≤ 0.040 ≤ 0.030 12.00 - 18.00 ≤ 1.00 58.00 - 66.00 - Fe: bal.
(9.4816)
Small abstract of all cast alloys of Otto Junker.