Sei sulla pagina 1di 7
luesresum | 2049 kon oa rm, ice 925mm rear | 05 moe ements: 025m 40a 050 050mm (050-ma ozt070 ‘025m 016. sr | suse ‘oaome | atom zess | 4nss ogame | 925m oaome | 0. max osommc se9| oso-00 note 2) 20m | 025m, 0.20 mmc (se9| 005-a20 Note 2) 015mm | 0200, Note 1 These alors arent roaly accept for aplcton in ec contac seater ote 3 tins cr=0 42.49, 050 ax aa0s A Nao 1) 0:38 me, 050 max (502 ae 2) 020 me. 030 mae (see Nae 3) 0,207 6 eae tet) 070m. 025m 06m one oso me. 020 ma. ozs ma 10 ma Table 8.1.3 Minimum mechanical properties for acceptance purposes of selected rolled aluminium alloy products: flloy andtemper | Thickness t mm 0-2%proot stress] Tenaie trenain]| — Gongation Elongation condi, see Note 3 Ry Ry ade | ons.e5f5, 50% New? Nome 5080 SstsSN(seentte2)| 25 0 6 4 see Hitt gete50 es 215-350 6 4 5000-112 gete50 es 28 2 0 5000-116 gete50 8 305 0 0 sone HZ 2etzo 15-208 305-380 w 0 5096.0 2etzo wo 240-08 6 “ 5086-111 2etzo wo 240-08 6 “ 5086-112 axteas. us 250 a - s25<1<60 5 240 - ° 5086-416 259 105 ms 10 (see Note 1) ® s0580 astsso 00 30 2m 24 sone astsso 00 30 2m 24 Sone-Ht16 asts20 zo 370 10 0 mo Group A: sumniumyagnesimaljs th lg conlert 535 per cent (ales $754) © Groups: slumnureragnestumalojs Wh 4 per cent slg 24.6 et cent (alojs 5053, S083, 5086, 5383 ana 5456), © Gtoup¢ aluminum ragnedumsiican ator (aloys 6005, 6061 and 6032), For sactg1cup, th quaestion made on one ay quash aocodure uth aha atysin to group, win eau or wor ‘ens stengh attr weking The qualfeaton made on arup Boys quafis the proceds for Group A aloys a0. Approval ir the ‘range of matt grades f surmised h Table 12. 5 una prs ich Table 12.4.4 Welding procedure approval, weldi positions for aluminium alloy s Test Position Positions Approved [Downhand D D onzomtatvertical x Dx Vertical up vu D.xvu Jovernead ° DX vuando Note Welcing invertical down (Vd) postion fs net roconmended. Table 12.4.5 Welding procedure approval, alumi jum material grades approved Matera usedin quaitcation test ‘Material Grades approved 5758 5758 5005 3005 | 5754 5083 3083 | s0se | 5754 5388 ‘a83_| 603s | 5068 | 5764 5069 5050 | 222 | S020 | 5085 | 754 5458 s450_| #382 | 083 | s0e0 | 754 0084 eons | €02 | 6061 5082 ‘e006 | 6082 | 6064 8061 eons | cos2 | 6001 ote Aprroval incluces all the diferent strained and termered conditions in each case Table 12.4.6 Range of qu n for parent material thickness Thickness of test assemtly, Range of qualficction| Range of quelfivation All sinde-run or two-run (T technique) butt welds O.stto 4,1¢ O5tto 1,1¢ Otto 1.10 Table 12.4.7 Range of qualification of throat thickness for fillet welds Throat thickness of test piece, a (rmm)] Range ot qualification la<10 OTs ato1sa Ja=10 275 ‘Table 19.8.1 Minimum mechanical properties for alum inium alloys oy conten 0285 ret cose, Ni Ute eneie arena, Won? Unveces | wees nelees Waeee| (osette 4) (esentes) poe omit 12 we a 2 soe ee 125 05 Ea 25 sae ont We 16 20 2 086 nie _ 0 6 20 “soone2) (seeNte2) 500 raven 195 5 25 2 050 eae 280 0 0 = sas o 125 5 8 25 Bese He ooo 20 (estos) ‘ : (ecenne 5) 51s ra Er m6 ws 2 (seenmes) (eeennes) a0 sire Girudee Open Prem ze 70 = 72 (soo Nato 1) traded Closed Profi 2 ‘00 20 40 se tate 1) Bruges open Prone 0 us 0 +0 Etude Closed Profi 205 15 25 veo 022 TSTe Roles 20 1 280 10 Bruges Open Prone 20 us x0 +0 Etude Closed Profi 240 15 20 v0 note 1. 1nase toys are net orm) acetate tor appicton in arct contact s-vsten om 2 sea eumelanin upon cs mh est Tn ote 3. The mechanical properties tobe usedto deter scartngs mathe pes and arades of suru aby manctactreé National or popietay Standards and pecicaons arto bo ividualy aged wihLR, 99 alo Oh 8 11 Scapa 115 Note 4. where deta srucuralanatrsic cried out unvoldod sresevalues maybe used! nay foment flecodzanes and vlines ove 90 P15. ca 2 13 Aum 3 of he Restor Sts. ote 5 Fer thictnesstess han 125 mr the mnirumunueies 0.2% prot sressisto be taken 25230 Nr andthe mrimumtensle rondnist be taken 26315 Nem. Table 11.9.1 Requirements for butt weld tests ‘insures Rapa Gate GooWeTe 1) | Base mebralvedTarie ea arenahninn? amimum | BenaTes rato (RRMIRWA eee “90 3 LaRCMRWCt 009 25 s LRCaNR NC? sommar 5ts6 20 s {ooo tote2) LRROMR NCR 059 20 4 ‘ecene2) ‘seetates) «81 1 4 2 0 4 Note + Tne pretses'R and W iaate Yor erm for Gas Tungsten AvcWelang (GTA oF we Ternor Gas Mea Are Weng (cua ana Grae ote 2 Approval et race LRRCALR WC2 confers approval ot 5383, S455 ana SIBS base meena rae ote 3 approval et race LRRCHLR NCS cntrs approval ot 5059, 5363, S456 ana SOBs base mana ra0e8 Note 4 Aporval of rade LRROALR WD confers aperoal of 005A, 8081 and C082 base movil grades Table 11.9.2 Shielding gas compositions sroue ‘Gascorpestin (val) (seetete) eu Argon a = 00 2 100 — 6 30805 emeincer s Special 28 ress, ote cacesot cher compaction rinse gate) or psc purty may be conser 2 pedal caee¢ ane wiles separa approval

Potrebbero piacerti anche