Sei sulla pagina 1di 3

CASE STUDY Project Crown

P & G
CCPL contractor
VEC consultant
KIRVY
LOYD
Designer kulvelka salkar

Stone dust

Antityrmite - chlorofyle (1 lt.) + Water (19 lt.) - 7 lt/sqm poured in holes in soling
Test Dry density
OMC
Slump cone test to check the workability at plant, expected value is b/w 55 to 100 for
making of slab on grade.
Bottom layer of soling two layers - 150 mm each
Reinforcement 10 mm dia. Bars all over
bottom layer 200 mm c/c, 30 mm cover
Upper layer 400 mm c/c, covers 40 mm
Steps of equipments used -
Niddle vibrator is used to make concrete homogeneous and to get rid of air voids. Duration
should not exceed 3-4 seconds at a particular point otherwise problem of segregation has to
face.
Screed to level the surface, vibrations are limited to surface only.
Aluminium strip
Vaccum dewatering
Hardening

Tolerance - 5 mm
50d overlap lap length
Slab thickness 230 mm
Cover blocks made up of 1:2 sand cement mixes (rich mix), 20 days curing.
Curing of slab 14 days continuous with gunny bag and then 7 days with the watering. Curing starts
after 12 hours in summer.
Channel removal after 2 days
Test for mix design Slump test & cube test
Cube test Core cutter test (if cubes fail) -- upv
12 trucks concrete in one strip.
SIKA (SIKA
R
Chabdur) hardener 6 kg/m
2
Asphalt chemical new technology (spray) after 15 days machine to get tough and shining slab

First safety
Second quality
Third schedule
Fourth cost

Total area of concreting 12500 sqm
Anti termite mixture of 1 lt. Chemical + 19 lt. Water

Trimix Flooring, also known as Vacuum Dewatered Floors but not necessarily. Trimix Flooring has
enormous advantage over the traditional concrete floors and has gained worldwide fame in a very
short span of time. Counting the major benefits of Trimix flooring, it increases the compressive
strength and the tensile strength of the floor by at least 60%. The abrasion resistance of the floor too
increases which minimizes the wear and the tear process. With Trimix Flooring Services, we can
down the cement consumption rate of many of the industries.

Admixture used 3.48 lt. (purpose is to do not get concrete set while transporting to the site used as
plasticizer)
0.4 void ratio
435 kg/m
3

Shalitex board at expansion joint
PVC pipe on dowel bar
CHECK LIST POINTS
1. Concrete delivery and pour record.
2. Check list of trimix panel.
3. Survilience observation
4. Reinforcement inspection checl list.
5. Inspection check list.
6. Quality surveillances for workmanship of concrete.
7. Post concrete inspection
Round disc -
Plate (purpose is to harden the concrete by mixing hardener properly) shaking
Blade (purpose is to make polishing concrete slab) rubbing
Broom finish is opposite of Smooth finish.
Sealant Grooving
Neto Bond is used for inner side Grouting.
Vacuum Dewatering -
Pump calibration 250-300 mm of Hg pressure
7.5 HP

Funti Aluminium strip
PEB pre engineering building
Type of vibration needle form 60 mm
If slurry is not removed then surface cracks generate.


PORTA Cabin
NCR non conformation report